Practical notes on optical brightener dosage in plastics, thermal degradation during extrusion, anti-yellowing performance and trial methods for masterbatch.

The extruder is the real test
A brightener can look excellent in a cold lab blend and fail after a twin-screw pass. Screw temperature, residence time, shear and the presence of regrind all add thermal history. Yellowing is often caused by the polymer or additives, with the brightener then asked to mask it — a losing strategy if the grade itself is degrading.
Start low, step up, measure
Most polyolefin applications start around 0.01%–0.05% by polymer weight. Run a stepped series (for example 0.01%, 0.02%, 0.03%, 0.05%) on your own resin, mould plaques at your normal temperature, and measure whiteness under a fixed light source. The curve will flatten at saturation — that is your ceiling, not a target.
Regrind changes the maths
Recycled content usually carries a yellow cast and may already contain brightener from the first pass. Increasing regrind ratio therefore changes both the required dosage and the achievable shade. If regrind is part of your formulation, test the actual blend, not virgin resin.
Dispersion beats dosage
Specks, streaks and uneven fluorescence usually come from poor dispersion rather than too little additive. Fine, consistent particle distribution and a compatible carrier in masterbatch are often more effective than increasing the loading. Check for plate-out on the screw and mould surface during longer runs.
What to ask your supplier
Ask for the thermal stability data at your processing temperature, a batch COA, a sample from the production lot (not a specially prepared lab lot), and confirmation of consistency between lots. Then approve on measured plaque whiteness and shade.
Questions & answers
Why does my white plastic part turn yellow after processing?
Common causes are excessive melt temperature or residence time, oxidation of the polymer, regrind content, and degradation of a brightener that is not rated for that temperature. Check the thermal history first, then confirm the grade's heat stability with your supplier.
Does adding more optical brightener always increase whiteness?
No. Fluorescence saturates. Beyond the optimum, additional brightener adds cost, can push the shade blue and may cause blooming or plate-out. Determine the optimum with a stepped dosage trial.